Discover the Power of Durability, Stability and Precision From Akuracy , a brand fully owned by Ratnakar Enterprises Jointly With Balaji Industries.

We offer high-quality products with unbeatable Innovative technologies and flexibility.

Our commitment to excellence is unmatched. Enjoy the benefits of our top-notch products today!

Hardness Conversion Charts: HRC to HV and HB Without the Common Mistakes

Akuracy Rockwell cum Brinell hardness tester used to measure HRC and HB values on steel parts

Ameet Kudche |

Short answer: a hardness conversion chart turns a reading on one scale (for example Rockwell C) into an approximate value on another (Vickers or Brinell). The tables in ISO 18265 and ASTM E140 are empirical. They were built from comparison tests on specific material groups, so they only hold for those materials and they always carry some uncertainty. Use them for guidance and process control. When a drawing or standard specifies a scale, test on that scale.

Akuracy Rockwell cum Brinell hardness tester used to measure HRC and HB values on steel parts

Why hardness scales don't convert exactly

Each method measures something different. Rockwell measures the depth of an indentation under a defined preliminary and total force. Vickers and Brinell measure the size of an indentation and divide force by surface area. The indenter shapes also differ: a diamond cone, a diamond pyramid and a ball. How a material responds to each depends on how much it work-hardens, its elastic recovery and its microstructure. Two steels with the same HRC can therefore show slightly different HV values. There is no physical formula that converts one scale into another for every material.

Which conversion table should you use?

  • ISO 18265: the international standard for converting hardness values for metallic materials. It has separate tables for different material groups, for example unalloyed and low-alloy steels and cast steel, steels for quenching and tempering, and some non-ferrous groups.
  • ASTM E140: the ASTM equivalent, with separate tables for non-austenitic steels, nickel alloys, cartridge brass, copper alloys and others.

Always name the table on the report, for example "converted per ASTM E140, Table 1". A converted value with no source is very hard to defend in an audit.

Approximate HRC to HV and HB values for steel

The table shows typical values from the ASTM E140 table for non-austenitic steels. Treat them as approximate and check the current edition of the table you cite.

Rockwell C (HRC) Vickers (HV), approx. Brinell (HB), approx.
20 238 226
30 302 286
40 392 371
50 513 Above the usual range for a steel ball; use a tungsten carbide ball (HBW) or another scale
60 697 Outside the Brinell range

The HV values grow much faster than the HRC values at the top end, so a one-point HRC difference near 60 HRC is worth far more HV than near 20 HRC. That is why converted values on hardened parts carry a larger spread.

Five common conversion mistakes

1. Using a steel table for non-ferrous metals

Aluminium, copper alloys and brass have their own tables, or none at all for some scales. Applying a steel chart to a brass bush gives a number that looks precise but means very little.

2. Converting outside the table range

Rockwell C is not meant for soft materials. A "converted" HRC below the bottom of the table should be reported on a suitable scale such as HRB or HBW. Brinell with a tungsten carbide ball (HBW) is limited to 650 HBW under ISO 6506-1, so very hard parts belong on HRC or HV.

3. Converting case-hardened or coated parts

A surface layer makes the reading depend on the indentation depth. A light Vickers load and a 150 kgf HRC test sample different depths, so their results can't be compared through a chart. Use a hardness traverse and report case depth instead.

4. Treating conversion as acceptance

If a specification says "250–320 HV", measuring HRC and converting may be fine for in-process checks. For the certificate, though, the customer may expect a real HV test. Agree this in advance.

5. Reporting without the original value

Good practice is to report the measured value and the scale first, then the converted value with the table reference. For example: "31.5 HRC (measured); ≈ 310 HV (converted, ASTM E140)."

Estimating tensile strength from hardness

ISO 18265 also includes approximate relationships between hardness and tensile strength for some steels. They are useful for a quick sorting check, such as spotting a wrongly heat-treated batch. They are not a substitute for a tensile test where a standard calls for one.

Equipment that reduces the need to convert

The simplest way to avoid conversion errors is to test on the specified scale. A combined tester helps labs that receive drawings calling for both Rockwell and Brinell. Akuracy's Rockwell cum Brinell hardness tester lists Rockwell test loads of 60, 100 and 150 kgf and Brinell loads of 187.5 and 250 kgf. For HV specifications, the Vickers hardness tester is listed with test loads from 5 to 50 kgf, 70X optical magnification and a 0.001 mm least count. You can compare other options in the hardness tester range.

Where this matters in industry

Heat-treatment shops report HRC but receive drawings in HV. Forging and casting suppliers are asked for HB but often check in HRC on the shop floor. Fastener makers work to property-class limits given in both HV and HRC. In each case, stating which value was measured and which was converted avoids disputes at incoming inspection.

FAQ

Is HRC to HV conversion accurate?

It is approximate. Conversion tables are empirical and depend on the material group, so a converted value carries more uncertainty than a direct measurement.

Which standard covers hardness conversion?

ISO 18265 internationally, and ASTM E140 in the ASTM system. Each has separate tables for different materials.

What is 30 HRC in HV?

About 302 HV for non-austenitic steel, according to the ASTM E140 steel table. Other materials will differ.

Can I convert Rockwell to Brinell for aluminium?

Only with a table made for that material group. Don't use a steel table.

Should I report converted hardness on a test certificate?

Only if the customer accepts it. Then report the measured value and scale first, and give the conversion table as the reference.